High-alloy steel – stainless low carbon high chrome steel H17PN-71 / H-86020
| Steel grade | Standard |
Chemical composition (%) |
|||||||||
| C |
Mn |
Si |
P |
S |
Cu |
Cr |
Ni |
Mo |
other |
||
| H17 | PN | max0,10 | max0,80 | max 0,80 | max 0,040 | max 0,030 | max 0,30 | 16,0018,00 | max0,60 | - | - |
| 12H1712KH1712Ð¥1712Ch17 |
GOST |
max 0,12 | max0,80 | max0,80 | max 0,035 | max 0,025 | max 0,30 | 16,0018,00 | max 0,60 | max 0,30 | V max 0,20 W max 0,20 Ti max 0,20 |
| X 6 Cr 17 X6Cr17 1.4016 |
DIN EN ISO W.nrEN |
max0,08 | max1,00 | max 1,00 | max 0,040 | max 0,015 | - | 16,0018,00 | - | - | - |
| X6Cr17EH4 |
ISO |
max 0,08 | max1,00 | max 1,00 | max 0,040 | max 0,030 | - | 15,00 17,00 | max 1,00 | - | - |
| Z 8 C 17 Z8C17 |
AFNOR |
max 0,08 | max1,00 | max 1,00 | max 0,040 | max 0,015 | - | 16,00 18,00 | - | - | - |
| S 43000S43000
430 |
UNS AISI |
max 0,12 | max1,00 | max 1,00 | max 0,040 | max 0,030 | - | 16,00 18,00 | - | - | - |
| 1Cr15
1Cr17 |
GB/T | max 0,12 | max1,00 | max1,00
max 0,75 |
max 0,035 | max 0,030 | - | 16,00 18,00 |
- max 0,60 |
- | - |
| SUS 430 SUS430 F SUS 430 FSUS430 |
JIS | max0,12 | max 1,00 | max 0,75 | max 0,040 | max 0,030 | - | 16,00 18,00 | max 0,60 | - | - |
Steel used in the production of machine parts, working in the nitric acid industry, in industries: dairy, beverage,
sugar, fruit and vegetable processing as well as catering facilities and in households.
Resistant to atmospheric corrosion, corrosion operation
-Natural water
-Steam
Cold, diluted organic acids (oxalic, malic acid, acetic acid - C 2 H 4 O 2 to 5% and more)
-Hot fumes of oil, especially containing sulfur, petrol and other fuels
-Food products (milk, edible oils, alcohol, cheese, etc.)
-Salt solutions
-Diluted solutions of alkali (sodium hydroxide to 20% with a boiling point up to 30% at normal temperature
ammonia in each concentration and temperature)
H17 steel is also resistant to intercrystalline corrosion
In grade H17 (1.4016, X6Cr17 or other substitute), we offer sheets, rods, forgings.